TCB Metal Works
Free Training

How to MIG Weld

MIG welding is the process most people learn first, and the one most fab shops run all day. This course takes you from an unplugged machine to a bead you can bend-test: what the parts do, how to stay safe, how to set the machine, how to hold the gun, and how to tell what went wrong.

Every number on this page comes from a published source: the U.S. Navy’s Steelworker training manual, OSHA, the American Welding Society, and the welding manufacturers Lincoln Electric, Miller, Hobart and ESAB. Small tags such as Miller name who says it. Where the sources give different numbers, we show the range and say who says what.

The Shop Card

The whole setup for mild steel on one table. Print it and hang it by the welder. Every line is explained further down.

ItemStarting point for mild steel, short circuitFrom
PolarityDC electrode positive (DCEP, reverse polarity) for solid wireMiller, Navy
WireER70S-6 on mill scale or dirty steel, ER70S-3 on clean steel. .030 in all-around, .023 in for thin, .035 in for thickerMiller, Lincoln
Gas75% argon / 25% CO2 (C-25)Miller, Lincoln, Navy
Gas flow20 to 35 cfh; the published ranges overlap at about 25 cfhMiller, Hobart, Navy
StickoutAbout 3/8 in of wire past the contact tip (3/8 to 1/2 in)Miller, Lincoln
Amps1 amp for every .001 in of thickness: 1/8 in steel = 125 AMiller, Hobart
Wire speedAmps × inches per amp for your wire (.030 in: 2 in per amp)Miller, Hobart
VoltageStart from the chart in the machine’s door. Wire stubbing into the plate: raise it. Erratic, spattering, burning back: lower itMiller, Hobart
Travel angle5 to 15°, pushing on solid wireMiller
Work angleButt 90°, T-joint 45°, lap 60 to 70°Miller
SoundSteady crackle, like bacon fryingMiller, Hobart
LensShade 10 minimum from 60 to 500 A; 11 to 14 suggestedAWS, OSHA

What MIG Welding Is

MIG stands for metal inert gas. The technical name is gas metal arc welding, or GMAW, and some people call it wire welding. A spool of solid wire feeds through a gun into the joint. An electric arc between the wire and the work melts both, and a shielding gas blowing out of the gun keeps the air off the molten metal. Miller

A welder in an auto-darkening helmet and gloves MIG welding a joint on a large pipe
MIG welding a joint on pipe: wire feeds through the gun, the arc melts it into the joint, and shielding gas covers the puddle. Photo: Weldscientist, Wikimedia Commons, CC BY-SA 4.0, resized.

There is no flux on solid wire, so a MIG weld is clean and there is no slag to chip off. Navy Miller says MIG handles most fabrication and repair welds from 24 gauge sheet up to 1/2 inch thick. Miller

The parts of a MIG welding setupA shielding gas cylinder chained upright with a regulator and flowmeter on top, a hose to the welding machine, a wire spool inside the machine feeding the gun cable to the MIG gun, and a work clamp lead from the machine to the part on the table.Shielding gasRegulator / flowmeterPower source and wire feederWire spoolGun cableMIG gunWork clamp lead
A MIG setup. Gas, wire and current all meet at the gun. The work clamp closes the circuit through the part. Schematic, not to scale.

The parts

  • Power source. A MIG machine is constant voltage: it holds the voltage you set, and the amperage follows the wire speed. Feed the wire faster and the current goes up; slower and it goes down. Navy, Miller
  • Wire feeder. Drive rolls push the wire from the spool, usually inside the machine, through the cable to the gun. Miller
  • Gun. Carries the wire, the current and the gas to the arc. At the front are the consumables: the contact tip, which guides the wire and passes the current into it, the diffuser, and the nozzle, which aims the gas at the puddle. Navy, Miller, ESAB
  • Gas. A cylinder with a regulator or flowmeter. On a typical regulator, one gauge shows cylinder pressure and the other the flow you set. Miller
  • Work clamp. Connects the part to the machine and closes the circuit. Miller

Safety First

A MIG arc burns eyes and skin, the fume is harmful, the sparks start fires, and the circuit can shock you. Set up right every time.

Labeled drawing of a safe MIG welding station: welder in helmet, jacket, gloves and boots, fume extraction hood, machine and secured gas cylinder
A safe MIG welding station: helmet, jacket, gloves and boots on the welder, fume extraction over the work, and the gas cylinder on the machine. Photo: Cierrex (original), Bernardwelds (handle), Curkuma Putz (composition), Wikimedia Commons, CC BY-SA 3.0, resized.

Eyes and skin

Never look at the arc without eye protection; it can do permanent damage. Bare skin near the arc gets painful burns. Navy Much of the arc’s light is ultraviolet, which you cannot see. It rises roughly with the square of the current, and argon-shielded processes like MIG give off more of it than most. AWS

Lens shades for MIG (GMAW) and flux-cored welding from the AWS lens shade selector, the same values OSHA prints in its eye protection fact sheet. OSHA’s older general table, 29 CFR 1910.252, lists shade 12 for gas-shielded arc welding on steel.
Arc currentMinimum shadeSuggested shade (comfort)
Under 60 A7Not listed
60 to 160 A1011
160 to 250 A1012
250 to 500 A1014
  • Pick the shade. AWS’s rule of thumb: start with a shade too dark to see the weld, then go lighter until you can see it, without going below the minimum. AWS
  • Safety glasses under the helmet, with side protection. Nearly 70 percent of eye injuries are caused by flying particles, and the helmet is up whenever you chip, grind or look over a weld. AWS
  • Check your auto-darkening helmet. Blocked sensors, dead batteries, a wrong sensitivity setting or a very cold shop can stop it from darkening. AWS
  • Protect the people around you. AWS measured how far UV carries from a MIG arc on mild steel with CO2 at 200 amps: about 7 feet for a 1 minute exposure and 23 feet for 10 minutes before it passes the daily limit. Bare metal and concrete floors reflect it. Use welding screens, but not blue see-through curtains, which do not block blue light. AWS

What to wear

  • Natural fibers: leather, wool or heavy cotton. They absorb UV better than synthetics, and heavy fabric is harder to light. AWS, ANSI Z49.1
  • Nothing that melts. No polyester, nylon, plastic or oilskin; melting fabric causes severe burns. AWS, Navy
  • Long sleeves, and cuffless full-length pants worn over the boots, not tucked in. Cuffs and open pockets catch sparks. AWS, Miller
  • Leather welding gloves, dry and without holes. ANSI Z49.1 requires flame-resistant gloves for all welders. AWS
  • Leather, safety-toed, high-top boots, and a cap or bandana under the helmet for the top of your head, more so overhead. AWS, Navy, Miller
  • Empty your pockets of butane lighters and matches. AWS

Fume and gas

The smoke from welding carries harmful metal fume and gases. Short exposure brings eye, nose and throat irritation, dizziness and nausea; long exposure to manganese fume can cause Parkinson’s-like symptoms, and welding fume is on the IARC list of cancer risks to humans. OSHA, AWS

  • Keep your head out of the plume. Heat makes it rise from the weld. Move the work or your head so you are not over it. AWS
  • Pull the fume away at the source. Keep hoods, fume extractor guns or vacuum nozzles close to the weld. Welding outdoors does not guarantee good ventilation; stay upwind. OSHA
  • Wear a NIOSH-approved respirator when ventilation is not enough. AWS
  • Shielding gas can suffocate you. Argon and CO2 push the oxygen out of a closed space. Never weld in a confined space without ventilation. OSHA
  • Clean off paint, solvent and coatings before you weld. OSHA
  • Galvanized steel: zinc fume is the most common cause of metal fume fever: headache, fever, chills, aches and nausea that start hours later and can last 6 to 24 hours. It is more likely after time away from the job. AWS
  • Stainless steel: welding turns its chromium into hexavalent chromium, which is highly toxic and causes cancer. OSHA

Fire

Sparks and spatter can travel up to 35 feet. AWS OSHA’s welding rule says to move combustibles at least 35 feet from the work where you can. Where appreciable combustible material is within 35 feet, a fire watch is required, and it stays for at least half an hour after the welding stops. OSHA 1910.252

  • Keep a fire extinguisher close and know how to use it. AWS
  • Things like wood dust can smolder for a long time, even days, before you see smoke. AWS
  • Never weld on a drum, tank or pipe that held something unknown or flammable until it has been made safe. AWS

Electric shock

Shock from welding equipment can kill. When the machine is on, the wire, the spool, the drive rolls and every metal part touching the wire are live. AWS

  • Wear dry gloves without holes and never touch the wire with a bare hand. Do not wrap the cables around your body. AWS
  • Clamp the work as close to the weld as you can. Never use a gas line or electrical conduit as the ground. AWS, OSHA
  • Check the input power cord often; replace it if it is damaged. AWS

Gas cylinders

  • Chain or strap the cylinder upright at all times, but not to a building member that could carry current. OSHA, Navy
  • Before you put on the regulator, stand to one side and crack the valve open and shut to blow out dirt. Open the valve slowly by hand. AWS
  • Take the regulator off and put the cap on before moving a cylinder, unless it is secured on a cart made for it. OSHA

Set Up the Machine

  1. Polarity. Solid MIG wire runs DC electrode positive, also called reverse polarity. The connections are usually inside the machine. Self-shielded flux-cored wire is the opposite: electrode negative. Miller, Navy
  2. Drive rolls. Match the roll to the wire: V-groove or knurled for solid steel wire, knurled V-groove for flux-cored wire, which is softer, and polished U-groove for aluminum. Contact tip, drive rolls and liner all have to match the wire diameter. Lincoln, Hobart, Miller
  3. Tension. Too much or too little tension on the drive rolls or the spool hub causes poor feeding; set it by your owner’s manual. Too much flattens the wire so it will not feed through the tip. Miller, Hobart
  4. Consumables. Clean spatter out of the nozzle, replace worn contact tips and liners, and throw out wire that looks rusty. Dirty or oily wire makes unsound welds. Miller, Navy
  5. Gas. Open the cylinder, set the flow (see the next lesson) and check the hose for leaks with soapy water. Miller
  6. Work clamp. On clean, bare metal, close to the weld. Miller, AWS
A wire feeder with a spool of welding wire, the drive system and the gun cable
A wire feeder: the spool of wire, the drive system that pushes it, and the cable out to the gun. Photo: Mgschuler, Wikimedia Commons, CC BY 3.0, resized.

Stickout

Stickout is the bare wire between the end of the contact tip and the arc. It does not include the arc. Miller says to hold about 3/8 inch; Lincoln gives 3/8 to 1/2 inch for short-circuit MIG and 3/4 to 1 inch for spray and pulsed. Miller, Lincoln

Wire stickout at the MIG nozzleClose-up of a MIG nozzle over a plate. The contact tip sits inside the nozzle. The wire sticks out past the end of the contact tip to the arc; that length, about 3/8 in, is the stickout. Shielding gas flows out of the nozzle around the arc and weld pool.Stickoutabout 3/8 inNozzleContact tipShielding gasFinished beadArcWeld pool
Stickout is the bare wire between the end of the contact tip and the arc. It does not count the arc itself. Schematic, not to scale.
  • Too long is one of the most common mistakes. More wire sticking out means more resistance and less current in the arc, and weaker gas coverage. The arc sounds irregular, and you get spatter and porosity. Miller’s rule: no more than 1/2 inch past the nozzle. Miller, Lincoln, Hobart
  • Too short and the wire fuses to the tip and shortens its life. Navy

The Navy manual measures stickout from the nozzle instead of the contact tip, so its figure of 3/8 to 3/4 inch is a different measurement. Navy

Pick the Wire and Gas

Wire

Mild steel MIG wire is named by its AWS class. In ER70S-6, the 70 means the weld has at least 70,000 psi tensile strength and the S means solid wire. Lincoln

A spool of copper-coated welding wire on its hub
A spool of copper-coated MIG wire on its hub. Too much or too little tension on the spool hub or the drive rolls makes the wire feed badly. Photo: AMPedNH, Wikimedia Commons, CC BY 2.0, resized. Credit: Desiree Crossley/Advanced Manufacturing Partnerships in Education/AMPed NH.
A shielding gas regulator with two gauges for MIG welding
A shielding gas regulator for MIG welding. Photo: Mimzy, Wikimedia Commons, CC0.
  • ER70S-3 is the most popular general-purpose wire. Lincoln, Miller
  • ER70S-6 carries more deoxidizers, silicon and manganese. It is the one for steel with mill scale, rust or dirt on it, and it wets out flatter at the edges. Lincoln, Miller
Amp ranges and inches of wire per amp from the Hobart / Miller Guidelines for Gas Metal Arc Welding. Uses from Miller’s mild steel basics.
Wire diameterAmp rangeWire speed per ampUsed for
.023 in30 to 90 A3.5 in per minuteThin material, less heat
.030 in40 to 145 A2 in per minuteGood all-around size
.035 in50 to 180 A1.6 in per minuteThicker material, more heat

Miller notes that a 115 volt machine may not have the output to run .035 inch wire on thicker steel, which risks cold lap. Miller Smaller wire is normal for vertical and overhead work. Navy

Gas

  • 75% argon / 25% CO2 (C-25) is the all-purpose gas for carbon steel: the least spatter, the best-looking bead, and less burn-through on thin metal. It costs more than straight CO2. Miller, Lincoln, Navy
  • 100% CO2 penetrates deeper but spatters more and leaves a rougher bead. The Navy says the current runs about 25 percent higher with it. Miller, Navy
  • 90% argon / 10% CO2 (C-10) and other argon-rich blends are for spray transfer on thicker plate. Miller, Lincoln
  • 100% argon is for aluminum. On steel it gives undercut, a poor bead shape and shallow penetration. Miller, Navy

Gas flow

The sources do not agree on one number for short-circuit MIG on steel: Miller gives 20 to 25 cubic feet per hour in one guide and 25 to 35 in another, Hobart 25 to 30, and the Navy about 35. The ranges overlap at about 25 cfh. Spray transfer takes more, 35 to 50 cfh. Miller, Hobart, Navy

More is not better. Too little gas leaves the puddle uncovered; too much wastes gas and stirs air into the shield. Both cause porosity. Miller Wind blows the gas away; Hobart says screens need to bring it down to 5 mph or less. Hobart Good shielding sounds like a crisp crackle or sizzle. A popping arc, discolored welds, porosity and spatter mean poor shielding. Navy

Set Wire Speed and Voltage

A MIG machine has two main knobs, and they do different jobs: Hobart, Miller

  • Wire feed speed sets the amperage, and amperage controls penetration. Too high can burn through.
  • Voltage controls the bead’s width and height.

Start from the door chart

Nearly every MIG welder has a settings chart, usually inside the door over the wire feeder, by material, thickness and wire size. Start there. Miller

Or use the rule of thumb

Miller and Hobart both use this one: 1 amp for every .001 inch of steel thickness. 1/8 inch steel is .125 inch, so about 125 amps. To turn amps into a wire speed, multiply by the inches of wire per amp for your wire size (table above). With .030 inch wire at 2 inches per amp, 125 amps is about 250 inches per minute. Miller, Hobart

Starting settings calculator

WireWire speed

Rule of thumb from Miller and Hobart. Set voltage from your machine’s chart, then tune both on scrap of the same thickness.

Fine-tune by eye and ear

  • Wire stubbing into the plate and pushing the gun back: the arc is set too short. Raise the voltage. Miller, Hobart, Lincoln
  • Arc erratic, spattering and burning back at the tip: voltage too high. Lower it. Miller, Hobart
  • Too little voltage also shows as a tall, convex bead that does not tie in at the edges, with extra spatter. Miller
  • Listen. A good short-circuit arc has a steady crackle, like bacon frying. Miller, Hobart

Always set up on scrap of the same thickness and joint before the real part. Hobart

Clean, Fit and Tack

Clean to bare metal

Solid MIG wire does not handle rust, dirt, oil or other contaminants well. Get grease and oil off first, then grind or wire brush down to bare metal before you strike an arc, and put the work clamp on clean metal too. Miller Oil, grease, mill scale, rust and moisture all cause porosity, and rust and mill scale add spatter. Hobart

The five joints

The five basic weld jointsEnd views of the five basic joints with the weld shown in orange: butt, T, lap, corner and edge.ButtT (tee)LapCornerEdge
The five basic joints, seen from the end. Orange is weld metal.

Edge prep and gap

  • Thin material, 0.035 to 1/8 inch: no edge prep needed; a gap (root opening) of 1/16 inch or less. Navy
  • 1/4 inch and thicker: bevel the edges so the weld goes all the way through, a single or double V with a 50 to 60° included angle. This matters most on butt joints. Navy, Miller

Tack welds

  • Tacks hold the parts in line until the final welds go in. The Navy puts them at 1/2 to 3/4 inch long, never more than 1 inch. Navy
  • A tack becomes part of the weld, so it has to be as good as the weld. Grind out cracked or porous tacks before welding over them. Navy

Fighting distortion

Weld shrinks as it cools and pulls the parts with it. Weld in short sections and let them cool in between, and keep heat down with lower settings or faster travel. You can also tack a T-joint slightly off square so the weld pulls it square. Hobart

Run a Bead

Get comfortable first

Use two hands on the gun and brace your hands, wrists or forearms so the gun moves smoothly. Take the weight of the cable and hose off the gun, across your shoulder if you need to. Miller, Navy

Close-up of a welding gun nozzle beside a fresh weld bead along a steel seam
A fresh weld bead along a seam, with the welding torch at the end of the bead. Photo: KOMATSU Ltd, Wikimedia Commons, CC BY-SA 2.1 jp, resized.

Travel angle: push or drag

Travel angle is how far the gun leans along the line of the weld. Miller calls for 5 to 15° in all positions; past 20 to 25° you get more spatter, less penetration and an unstable arc. Miller

Push and drag travel anglesTwo side views. Push: the gun leans back and points ahead in the direction of travel, 5 to 15° from vertical. Drag: the gun leans forward and points back at the finished weld, 5 to 15° from vertical.Push (forehand)5 to 15°Direction of travelGun points ahead, toward unwelded metalDrag (backhand, pull)5 to 15°Direction of travelGun points back, at the finished weld
Travel angle is measured from straight up and down, along the line of the weld. The bead runs left to right in both views.
  • Push (gun pointing ahead): a wider, flatter bead with less penetration, and a better view of the joint. The usual choice with solid wire, but too much push angle cuts penetration. Miller, Hobart
  • Drag (gun pointing back at the weld): deeper penetration and a narrower, taller bead. Miller
  • On steel either works. On aluminum, push only. With flux core, drag: “if there’s slag, you drag.” Miller

Work angle

Work angle is the gun’s angle across the joint, looking down the weld. Miller

Work angles for butt, T and lap jointsThree end views looking down the weld. Butt joint: gun at 90° to the plate. T-joint: gun at 45°, splitting the corner. Lap joint: gun at 60 to 70° measured from the bottom plate.Butt joint90°T-joint (fillet)45°Lap joint60 to 70°
Work angle is measured across the joint, looking down the length of the weld.
  • Butt joint: 90°, straight into the joint.
  • T-joint: 45°, splitting the corner evenly.
  • Lap joint: 60 to 70°; the thicker the metal, the greater the angle. Miller
  • Different thicknesses: angle toward the thicker piece. Navy
  • Horizontal fillets: drop the work angle another 0 to 15° to fight gravity. Miller

Travel speed

Keep the arc on the leading edge of the puddle. Miller, Navy Too fast gives a narrow, humped bead that does not tie in at the edges or penetrate. Too slow piles on heat: a wide bead, poor penetration, and burn-through on thin metal. A bead does not need to be bigger than the thinnest piece you are welding. Miller

Weaving

A single straight stringer bead does most narrow joints. Weave, or run several stringers, to fill a wide joint or bridge a gap, and pause slightly at each side of a weave to avoid undercut. Hobart, Miller

Starting and stopping

  • If the wire sticks to the work, let go of the trigger and clip it with side cutters. Navy
  • At the end of a bead, pause with the trigger still pulled and back up slightly to fill the crater. Hobart
  • Then hold the gun over the end until the metal freezes, so the gas covers it. Pulling away early causes crater porosity. Hobart, Navy

Welding Out of Position

Learn in the flat position first; the skill carries over. Navy Once you leave flat, gravity is working against the puddle:

A welder in an auto-darkening helmet MIG welding overhead
MIG welding overhead, one of the out-of-position welds covered in this lesson. Photo: Prowelder87, Wikimedia Commons, CC BY-SA 4.0, resized.
  • Turn it down. Miller suggests cutting voltage and amperage 10 to 15 percent from your flat settings for vertical; the Navy says about 10 percent less amperage out of position. For overhead, Miller gives at least 10 to 15 percent in one guide and 15 to 20 percent in another. Miller, Navy
  • Vertical up (start at the bottom, weld upward) penetrates better on thicker material, typically 1/4 inch and more. Tip the gun 5 to 15° down from square to the joint. Miller
  • Vertical down (start at the top) travels faster and penetrates less, which helps on thin metal. Miller
  • Overhead: travel fast enough that the metal does not fall out of the joint, keep any weave narrow, and wear a cap under your helmet. Miller, Navy

Transfer Modes

“Transfer mode” is how the melted wire crosses the arc into the puddle. Settings, wire and gas decide which one you get. Short circuit is the low-heat mode and the one to learn first. Lincoln

ModeHow the metal crosses the arcPositionsWhere it fits
Short circuitThe wire touches the puddle and shorts out, 20 to 200 times a second. Low heat.AllSheet and thin plate: Lincoln gives 0.024 to 0.20 in. Most shop and home MIG welding.
GlobularLarge drops form and fall by gravity. Hard to control, heavy spatter.Flat and horizontalUsually pure CO2. Hobart limits it to 1/8 in and thicker.
SprayA fine stream of small drops; the arc burns without shorting.Flat and horizontal on steel1/8 in and thicker. Needs argon-rich gas: under 18% CO2 (Lincoln), at least 80% argon (Miller).
Pulsed sprayThe machine switches between a high peak and a low background current.AllSpray-type welds with a smaller puddle. The machines cost more.

Lincoln and ESAB give 20 to 200 short circuits a second; Hobart gives 90 to 200. Spray transfer can put 98 percent or more of the wire into the weld, but its fluid puddle keeps it to flat and horizontal work on steel. Lincoln, ESAB, Hobart, Miller

Fix Bad Welds

Most bad welds come down to a few things: settings, gun angle, travel speed, stickout, gas coverage and dirty metal. Change one thing at a time. Miller, Hobart, Navy

What you seeLikely causesWhat to change
Porosity: pinholes or bubbles in the weldPoor gas coverage (flow too low or too high, wind, a spatter-clogged nozzle, a hole in the liner, stickout too long). Oil, rust, mill scale or moisture on the steelCheck the flow and hose, clean the nozzle, block the wind, shorten the stickout, clean to bare metal
Crater porosity at the end of the beadPulling the gun and its gas away before the crater setHold the gun over the end until the metal freezes
Lack of fusion (cold lap): the weld sits on topCurrent too low (the most common cause), wrong gun angle, wrong travel speedMore wire speed or voltage; 0 to 15° gun angle with the arc on the leading edge of the puddle
Burn-throughToo much heat; most common under 1/8 inLess wire speed or voltage; travel faster
Undercut: a groove melted beside the weldVoltage too high with travel too fast; arc aimed at the bottom plateLower voltage, slow down, aim more at the top plate
Ropey, convex beadWire speed too high for the voltageRaise voltage or lower wire speed
Flat, concave bead (flat or horizontal)Voltage too high, wire speed too low, or travel too fastLower voltage, raise wire speed or slow down
Heavy spatterVoltage too low for the wire speed (the most common cause), wire speed too high, stickout too long, 100% CO2, a worn or wrong contact tipRaise voltage, shorten stickout, try mixed gas, change the tip
Wire stubbing into the plateVoltage too low: the arc is set too shortRaise voltage
Bird-nest: wire tangles at the drive rollsWrong drive rolls or tension; a blocked, badly trimmed or wrong-size linerFlip up the drive roll, pull the wire back out of the gun, fix the cause
Burnback: wire welds itself to the contact tipWire speed too slow, or the gun held too closeReplace the tip; raise wire speed; keep your stickout
CracksWeld too small, joint held too rigidly, poor joint design, fast cooling, unfilled cratersSize the weld right, fill the crater, avoid over-restrained joints

Check Your Work and Practice

What a good bead looks like

  • Slightly crowned, with the edges (the toes) flowing smoothly into the base metal. Miller
  • Even width and height the whole length, with no craters or holes. Miller

Break it

A weld can look fine and still sit on top of the metal. Clamp a practice weld in a vise and bend it until it breaks. The metal next to the weld should break before the weld does. Miller The Navy lists three field tests that need no lab: the free-bend, guided-bend and nick-break tests. A nick-break shows the inside of the weld: gas pockets, inclusions and lack of fusion. Navy

You can also cut a practice weld across, polish the cut face and etch it. The etch shows where the weld metal ends and the base metal starts, so you can see how deep it went. Navy

Practice

Start in the flat position. Run beads and change one thing at a time, angle, speed, stickout or a setting, and watch what each change does to the bead. That is how you learn to read the puddle. Miller, Navy Then move to T-joints and lap joints, break them, and only then go out of position.

Getting certified

The American Welding Society’s Certified Welder program tests welders on procedures used in structural steel, pipeline, sheet metal and refinery work. It is a performance test with no required classes beforehand: you weld a test piece, an AWS Certified Welding Inspector checks it, and if you fail you can retest at any time. AWS

Flux Core, Aluminum and Stainless

Self-shielded flux core

Same machine, different wire. Flux-cored wire is hollow and carries its own shielding, so self-shielded wire needs no gas bottle, which makes it the better choice outdoors or in wind. Miller

A welder at a welding table MIG welding stainless steel with the machine beside the table
MIG welding stainless steel. Photo: Mgschuler, Wikimedia Commons, CC BY 3.0, resized.
  • Electrode negative (straight) polarity, knurled drive rolls, and about 3/4 inch stickout, roughly twice MIG. Miller, Hobart
  • Drag the gun. It leaves slag that has to be chipped off. Miller
  • E71T-11 is a general purpose, all-position flux-cored wire for mild steel. Miller

Aluminum

Aluminum conducts heat about six times faster than steel and melts at a lower temperature, so it warps and burns through easily, and it takes a faster travel speed. Miller

  • 14 gauge and heavier; thinner than that takes pulsed MIG or AC TIG. Miller
  • 100% argon, 20 to 30 cfh. Never a CO2 blend. Miller
  • The wire is soft, “like pushing a wet noodle through a straw.” Use a spool gun, or polished U-groove drive rolls with a Teflon liner and a straight cable. Miller, Lincoln
  • Degrease, then brush off the oxide with a stainless brush kept only for aluminum. Miller
  • Push only, 10 to 15° (Miller) or 5 to 10° (Lincoln). Dragging leaves gray or black, dirty welds. Spray transfer is the preferred mode. Miller, Lincoln
  • ER4043 and ER5356 are the common wires. 4043 is the easier one to weld; 5356 is stronger and resists corrosion better. Miller

Stainless

  • Common base metals are 304 and 316; common wires are 309 and 316. Miller
  • Keep CO2 low. Lincoln names 90% helium / 7.5% argon / 2.5% CO2 as the most popular short-circuit blend for stainless, and Miller says blends should stay at 5% CO2 or less. Lincoln, Miller
  • Use drive rolls and a liner kept only for stainless, so steel does not contaminate the weld. Miller
  • Stainless fume carries hexavalent chromium. Pull it away at the source. OSHA

Check Yourself

Answer each question in your head, then tap it to check.

1. Your solid-wire MIG welds are full of pinholes. Name three things to check.

Anything that hurts gas coverage or adds dirt: the gas flow (too low or too high), a leak in the hose or liner, wind, a spatter-clogged nozzle, stickout that is too long, and oil, rust or mill scale on the steel.

2. What polarity does solid MIG wire run on? What about self-shielded flux core?

Solid wire: DC electrode positive (reverse polarity). Self-shielded flux core: DC electrode negative (straight polarity). The change is usually made inside the machine.

3. About how many amps for 3/16 in steel, and which wire?

3/16 in is .1875 in, so about 188 amps by the 1 amp per .001 in rule. That is past the top of both the .030 in range (145 A) and the .035 in range (180 A) in Hobart’s table. Miller’s answer for thicker steel is .045 in wire, if your machine can run it. Check the door chart, and test on scrap.

4. The wire keeps stubbing into the plate. Which knob?

Voltage. Raise it. Stubbing means the arc is set too short for the wire speed.

5. Push or drag with solid wire on steel? With flux core? With aluminum?

Solid wire on steel: either works, and a push is typical; it gives a flatter bead and a better view. Flux core: drag (if there’s slag, you drag). Aluminum: push only.

6. What gun angles for a T-joint fillet?

A 45° work angle, splitting the corner, plus 5 to 15° of travel angle. If one piece is thicker, angle toward the thicker piece.

7. How do you end a bead without leaving a crater?

Pause at the end with the trigger still pulled and back up slightly to fill the crater, then hold the gun over it until it freezes so the gas keeps covering it.

8. Why do galvanized parts need extra care?

The zinc burns off as fume, and zinc fume is the most common cause of metal fume fever. Keep your head out of the plume and pull the fume away with extraction, or wear a respirator.

9. How far can sparks travel, and how long does a fire watch stay?

Up to 35 feet. Move combustibles at least 35 feet away where you can. Where a fire watch is required, OSHA says it stays at least half an hour after the welding stops.

10. Your practice T-joint is in the vise. What do you want to see when you bend it?

The metal next to the weld should break before the weld does. If the weld lets go first, it did not fuse in: the settings were too cold, or the gun angle or travel speed was off.

Sources and Limits

Read on November 24, 2026:

  • U.S. Navy, Steelworker, Volume 1 (NAVEDTRA 14250, 1996): welding safety and the gas metal arc welding chapter. Public domain.
  • OSHA (osha.gov): 29 CFR 1910.252 (welding, including its lens shade table and fire prevention), 1926.350 and 1926.351; fact sheets Controlling Hazardous Fume and Gases during Welding and Eye Protection against Radiant Energy during Welding and Cutting.
  • American Welding Society (aws.org): Safety and Health Fact Sheets 1, 2, 5, 6, 7, 25, 26, 30, 31, 33, 34 and 36; ANSI Z49.1:2012 Safety in Welding, Cutting, and Allied Processes; Certified Welder program FAQ.
  • Lincoln Electric, Gas Metal Arc Welding: Product and Procedure Selection.
  • Hobart / Miller, Guidelines for Gas Metal Arc Welding (GMAW); Hobart Brothers technical articles on MIG and self-shielded flux-cored troubleshooting.
  • Miller Electric knowledge hub articles: MIG basics for mild steel, tips for beginners, setting parameters, shielding gas, troubleshooting, common defects, flux-cored basics, solid vs flux-cored wire, pulsed MIG, automotive repair, aluminum and stainless.
  • ESAB, beginner’s guide to MIG welding.

Limits. This is a training course, not a welding procedure. Work that has to meet a code, such as AWS D1.1 for structural steel, is welded to a written procedure by a qualified welder, and that governs over anything here. Settings are starting points that change with the machine, wire, gas, joint and position. Where the sources disagree we give the range rather than pick one. The Navy manual dates from 1996 and the ANSI Z49.1 copy we read is the 2012 edition; check the current rules for your workplace. TCB Metal Works is not affiliated with any manufacturer named here. Product names belong to their owners.

Have a Project?

Talk to Our Team

Our specialists are happy to answer your questions and help scope your project.