TCB Metal Works
Free Guide

Metal Finish & Material Selection Guide

Two questions sit behind every fabrication: what should it be made of, and what goes on it afterward. The answers depend on each other, and both depend on where the piece will spend its life. This guide takes the choices in the order we would work through them.

Where a number or a claim appears, it comes from a trade association, a government agency or a producer, named at the end. Where something is our own shop practice, we say so.

Start With Where It Lives

Water and salt are what drive corrosion, so the first question is how wet and how salty the place is.

  • Indoors, dry and heated. The mildest exposure there is. UK steel construction guidance puts it in the lowest corrosion category, C1, and says no corrosion coating is required there. Paint or powder coat indoors is for appearance.
  • Outdoors, away from salt. Rain, dew and sun. Bare carbon steel rusts; coated steel does well.
  • Near salted roads, walks and parking. This is the one that matters most in Wisconsin. De-icing salt is very corrosive to construction materials, and it travels: traffic throws it into the air as a fine mist, and salt has been found up to 1.2 miles downwind of busy roads.
  • Washdown and chemicals. Kennels, food areas, zoo holding. Frequent wetting plus cleaners.
  • Coast and salt water. Not our local problem, but the same chemistry as road salt, all year.

For a local reference point, the American Galvanizers Association lists Milwaukee among its test cities and puts its measured zinc corrosion rate in the middle category, ISO C3. It also notes that most places in North America do not go above C3. Road salt right next to the steel is a harsher, local condition on top of that.

The Metals, Side by Side

Carbon steelStainless steelAluminumWeathering steel
Needs a finish outdoors?YesNo. The chromium in it forms its own protective layerOften not. It forms its own oxide filmNo. It is meant to rust to a stable layer
Main strengthStrong, cheap, easy to weld and formStays clean with no coating to chipAbout one-third the weight of steel, and resists corrosion bareNo coating to maintain
Watch out forRusts wherever the finish is brokenSalt stains the common grade; needs clean fabricationLoses strength next to weldsSalt, constant damp, and rust stains on what is below it
Read moreCarbon steelStainless steelAluminumWeathering steel

Carbon Steel

Most of what a fab shop builds is carbon steel. It is strong, it costs the least, it welds and forms easily, and it comes in every shape. Its one weakness is rust, which is why the finish sections below are mostly about carbon steel.

Common grades

Different products are made to different specifications. These are the ones behind most structural and miscellaneous steel:

ProductCommon specificationMinimum yield strength
Plate, and most angleASTM A3636 ksi (plate up to 8 in thick)
Wide flange beams (W shapes)ASTM A99250 ksi
Square, rectangular and round tube (HSS)ASTM A500 Grade B or C; most is made to meet both46 ksi for Grade B rectangular, 50 ksi for Grade C
PipeASTM A53 Grade B35 ksi

Note that pipe and tube are not the same thing. Tube made to A500 is a good deal stronger than pipe made to A53, and the Steel Tube Institute recommends keeping A53 pipe for nonstructural uses. Yield values are from the American Institute of Steel Construction and the Steel Tube Institute.

Hot rolled, cold rolled, pickled and oiled

  • Hot rolled steel has a rougher surface and carries mill scale, the dark scale left from cooling. Plate, beams, angle and most tube are hot rolled.
  • Pickled and oiled is hot rolled sheet with the scale removed in acid and a film of oil put on.
  • Cold rolled is rolled again without heat for a smoother surface. It is common in thinner sheet.

Mill scale matters for finishing. It is a poor base for a high performance coating and has to come off first, by blasting for paint and powder coat. Galvanizing takes it off in the acid bath as part of the process.

Hot-Dip Galvanizing

The finished steel fabrication is cleaned and dipped in a kettle of molten zinc. The zinc reacts with the steel and forms alloy layers bonded to it, with zinc on top. It coats everything the liquid reaches, including the inside of tube.

How it protects

Two ways at once. The zinc seals the steel off from the weather, and zinc also corrodes in place of steel. That second part is what sets it apart from paint: where the coating is scratched or cut, the zinc around the damage keeps protecting the bare steel. The American Galvanizers Association says a bare spot up to 1/4 inch across will not start to corrode until the zinc around it is used up.

How long it lasts

The same association says properly specified galvanized steel can give 70 years or more without maintenance in most atmospheres, depending on temperature, humidity, pollution and salt in the air. It measures life to “first maintenance”, the point where 5 percent of the surface shows rust. Life is in direct proportion to the zinc thickness, and thicker steel takes a thicker coating:

Minimum average zinc thickness under ASTM A123, as published by the American Galvanizers Association. One mil is one thousandth of an inch. These are minimums; the specification sets no maximum.
Steel thicknessStructural shapesPlatePipe and tube
Under 1/16 in1.8 mils1.8 mils1.8 mils
1/16 to under 1/8 in2.6 mils2.6 mils1.8 mils
1/8 to under 1/4 in3.0 mils3.0 mils3.0 mils
1/4 to under 5/8 in3.9 mils3.0 mils3.0 mils
5/8 in and over3.9 mils3.9 mils3.0 mils

Bolts, nuts and other hardware are galvanized to a separate specification, ASTM A153. Road salt is hard on galvanizing, as it is on other coatings, so the general figure does not carry over to steel that gets salted directly.

What it looks like

Fresh galvanizing can be bright and shiny, spangled, matte gray, or a mix of those on one piece. The chemistry of the steel affects it, silicon and phosphorus most of all. Appearance has no bearing on protection, and over time all of it weathers to an even matte gray as the surface layer forms, usually within 6 to 12 months. If an even look matters on day one, galvanizing alone is the wrong finish; see galvanizing plus a top coat.

Pieces stacked wet and tight right after galvanizing can grow a bulky white deposit called wet storage stain. In most cases it is light and does not shorten the life of the coating.

What it asks of the design

  • Vent and drain holes. Every closed tube and pipe needs them, so the cleaning solutions and the zinc can get in and back out. Liquid trapped in a sealed space flashes to steam in the kettle and can rupture the piece. On handrail, the association calls for holes at least 3/8 inch across, as close to the weld as possible. Our free galvanizing vent hole finder marks them on a STEP file.
  • Size. The piece has to fit the kettle. The average kettle in North America is 40 feet long. Longer pieces can sometimes be dipped one end at a time.
  • Distortion. The heat of the kettle can change the shape of a piece. Best practice is to keep pieces symmetrical and of similar thickness; a piece that mixes thin and heavy steel is the one at risk.

Powder Coating

Dry powder is sprayed on with an electrostatic charge that makes it cling to the grounded part. The part then goes into an oven, typically 375 to 400 degrees F, where the powder melts, flows and cures into a hard film. There are no solvents in it.

How it protects

As a barrier only. Powder on bare steel keeps water and air off the steel as long as the film is whole. When the film is breached by a scratch, a chip or a pinhole, the exposed steel rusts, and rust can spread under the film from there. There is no zinc to step in. That is the main difference from galvanizing. Our view is that powder coat over bare steel belongs indoors, or outdoors where a chip will be seen and touched up.

Which powder

  • Polyester powders hold up in sunlight and are the usual choice outdoors.
  • Epoxy powders are tough and resist corrosion well, but they chalk in sunlight. The Powder Coating Institute does not recommend epoxies or epoxy hybrids outdoors where looks matter.

What decides how long it lasts

What happens before the powder goes on. The steel is cleaned and given a pretreatment that helps the powder grip: iron phosphate is the most common, and zinc phosphate is used where the highest performance is needed. The Powder Coating Institute says powder can outperform liquid paint when it is applied to a properly pretreated part.

Limits

The part has to fit the spray booth and the curing oven. Powder coats what the spray can reach, so the inside of a closed tube stays bare.

Liquid Paint

Paint is still the answer for pieces too big for a kettle or an oven, for work finished on site, and for repainting. Like powder, an ordinary paint film is a barrier only.

Surface preparation comes first

Surface preparation is generally accepted as the most important factor in how long a paint system lasts. The U.S. Bureau of Reclamation, citing the Federal Highway Administration, puts up to 80 percent of early coating failures on bridges down to poor surface preparation or application. The paint industry grades preparation in levels:

LevelNameWhat is left on the steel
SSPC-SP 2Hand tool cleaningLoose mill scale, loose rust and loose paint are gone. Tight mill scale and tight rust stay.
SSPC-SP 3Power tool cleaningThe same result as hand tools, done with power tools.
SSPC-SP 6Commercial blastAll rust, mill scale and paint removed. Stains or shadows allowed on up to 33 percent of each area.
SSPC-SP 10Near-white blastAll rust, mill scale and paint removed. Stains allowed on only 5 percent of each area.

Hand tools such as scrapers and wire brushes do little against mill scale or tight rust. A paint specification that names a blast level is asking for the scale to be gone.

Paint systems

Long-life paint on steel is built in layers. The system used on steel bridges is a zinc-rich primer over blasted steel, then one or two coats on top. The zinc in the primer protects the steel the way galvanizing does, by corroding first. The middle coat is the barrier, and the top coat takes the sunlight and gives the color. The Federal Highway Administration reports that some three-coat systems with zinc-rich primers last up to 30 years before a major touch-up.

A single coat of shop primer is something else. It is there to keep blasted steel from rusting until the real paint goes on. It is not a finish.

Galvanizing Plus a Top Coat

Galvanizing can be painted or powder coated. The trade calls it a duplex system. The zinc gives the long-term protection, and the top coat adds color and another barrier. The American Galvanizers Association says the pair can last 1.5 to 2.3 times the combined lifetimes of the two coatings on their own.

The zinc surface has to be prepared or the top coat will not stick. ASTM D6386 covers preparation for paint and ASTM D7803 covers it for powder coating. A light sweep blast is the most common method, done with care because zinc is soft.

It suits outdoor railings, gates and architectural steel that have to be a color and have to last.

The Finishes, Side by Side

Hot-dip galvanizingPowder coatLiquid paintGalvanizing plus a top coat
How it protectsA zinc layer that seals the steel and also corrodes in its placeA sealed film. Barrier onlyA sealed film. Barrier only, unless the primer is zinc-richBoth: zinc underneath, sealed film on top
When it gets scratchedThe zinc around the scratch keeps protecting the bare spotThe bare steel rusts and the rust can creep under the filmThe same as powder coatThe zinc underneath still protects
LookSilver to gray, uneven when new, dulls to an even matte grayAny color, smoothAny colorAny color
Inside of tubeCoated, inside and outNot coatedNot coatedZinc inside and out; color outside
Size limitThe galvanizer’s kettleThe spray booth and curing ovenNone; can be done on siteBoth of the first two
Fits bestOutdoor steel where long life matters more than colorIndoor work, and outdoor work where a chip can be seen and touched upLarge pieces, field work and repaintingOutdoor work that needs both color and long life

Stainless Steel

Stainless steel is iron with at least 10.5 percent chromium. The chromium forms a thin oxide layer on the surface, called the passive layer, and that layer is the protection. There is no coating to chip, and the layer re-forms by itself on a clean surface in air.

304 or 316

  • Type 304 is the basic grade: 18 percent chromium, 8 percent nickel. It is the most readily available grade and the one usually specified for general-purpose work.
  • Type 316 is 304 with 2 to 3 percent molybdenum added. The molybdenum is what resists chlorides, meaning salt.

The International Molybdenum Association says that within five to ten miles of a large body of salt water, or where the steel is exposed to de-icing salt, Type 316 is often the most cost effective choice if corrosion-free performance is wanted. De-icing salt causes at least surface staining on Type 304. For a stainless railing along a salted walk or road in Wisconsin, that points to 316 with a smooth finish.

The L grades

304L and 316L are the low carbon versions: 0.030 percent carbon maximum, against 0.08 percent for the standard grades. They were developed to prevent a kind of corrosion beside welds, called weld decay. For welded work, the L grade is the one to ask for.

Finish and upkeep

Smoother is better. The British Stainless Steel Association says the smoothest surface always gives the best corrosion resistance, in any environment. Rougher surfaces stain more easily. The brown surface staining that shows up near salt is called tea staining. It is cosmetic and does not affect the strength or the life of the steel, and a light, regular wash keeps it down. Rain may be enough where it can reach.

The most common mill finish on cold rolled stainless sheet is called 2B.

Fabrication matters more than with carbon steel

  • Contamination. The Specialty Steel Industry of North America calls it the number one problem in stainless fabrication. Carbon steel particles from shared tools, grinding dust or forks get embedded in the surface and rust, so the stainless looks as if it is rusting.
  • Heat tint. The colored band beside a weld is a thickened oxide layer, and the metal under it has lost some corrosion resistance. Brushing may take off the color without removing that weakened layer; pickling or proper abrasive cleaning does.
  • Galling. Stainless threads can seize as they are tightened, a kind of cold welding. Lubricating the threads before assembly is the usual prevention.

Aluminum

Aluminum weighs about one-third as much as steel and resists corrosion without a coating. A protective oxide film forms on it in air, and for many uses that film is all the protection it needs.

Alloys

  • 6000 series alloys are the most popular for extrusions: tube, angle, channel and bar. Within the family, 6063 is the one often called architectural aluminum, and 6061 is the stronger one with the better strength for its weight.
  • 5000 series alloys are produced mainly as sheet and plate.

Welding costs strength

This is the thing to know before choosing aluminum for a welded structure. 6061-T6 has a typical tensile strength of 45 ksi as purchased. After welding, the structural welding code for aluminum, AWS D1.2, requires only 24 ksi, because the heat of welding changes the metal beside the weld. A welded aluminum frame has to be designed around the weakened zones, not the strength on the mill certificate.

Finishes

Aluminum can be left bare, anodized, painted or powder coated. Anodizing is not a coating put on the surface. It builds a layer of aluminum oxide out of the surface itself, so the finish is part of the metal and not a layer sitting on top.

Weathering Steel

Weathering steel, often called by the trade name Cor-Ten, is alloyed so that its rust forms a tight layer that slows further rusting. It is used bare. The specifications are ASTM A588 for structural shapes and A847 for tube.

The protective layer only forms with repeated wetting and drying. That makes it a poor choice in a few places:

  • Near salt. Salt holds moisture on the surface and keeps it damp, and chlorides are in every de-icing agent. Coastal air is ruled out for the same reason.
  • Where it stays wet. Against the ground, in standing water, where dew or plants touch it, and inside hollow sections where condensation collects.
  • Above anything you want clean. Rust runs off it and stains the materials below. Highway guidance is to protect the concrete under it and keep dirt and debris from collecting on it.

Most published guidance on weathering steel is written for highway bridges. For a planter, a sign or a screen wall the same rules apply: let it dry, keep salt off it, and plan for the runoff.

Mixing Metals

When two different metals touch and get wet, one corrodes faster and the other is protected. The metals are ranked in what is called the galvanic series. The more active metal of the pair is the one that suffers. Zinc and aluminum are at the active end, carbon steel is in the middle, and stainless steel is at the noble end.

The size of each piece matters as much as the ranking. A small piece of the active metal joined to a large area of the noble metal corrodes fast. The classic mistake is carbon steel bolts in a stainless railing: the bolts are the small, active part, and they rust away. The other way round, stainless fasteners in a large galvanized or aluminum part, is much less of a problem, and the American Galvanizers Association says contact between galvanized steel and stainless or aluminum is unlikely to cause much added corrosion in mild to moderate conditions.

  • Match the fasteners to the more noble metal, not the cheaper one. Do not use galvanized fasteners to join stainless.
  • Isolate where the conditions are wet or salty. An insulating barrier between the two metals, such as inert washers, is usually enough.

Details That Protect the Finish

A finish is easier to protect on the drawing than in the paint booth.

  • Pick the finish first. Galvanizing needs vent and drain holes and a piece that fits the kettle. Powder coat needs a piece that fits the oven. Both are cheap to allow for at the start and expensive to fix later.
  • Do the welding before the coating. Our practice is to build from bare steel and coat the finished piece. Welding on galvanized steel means removing the zinc at the weld first, working with good ventilation, and repairing the coating afterward. The repair standard, ASTM A780, allows zinc-rich paint, zinc solder or sprayed zinc.
  • Do not trap water. Open-top channels, pockets and unsealed laps hold water and salt against the steel. Give water a way out.
  • Plan the field joints. Bolted site connections keep the shop finish whole. Field welds burn it off and need a coating repair on site.

Where We Would Start

These are starting points, not rules. Every one of them can change with budget, looks and how the piece is used.

The jobWhere we would startWhy
Indoor railing, furniture, fixturesCarbon steel, powder coated or paintedDry indoor air is the mildest exposure, so the finish is for looks and wear.
Outdoor handrail or guard along a salted walkCarbon steel, galvanized. Add powder coat or paint over it if it has to be a colorZinc keeps protecting at scratches, and salt finds every chip in a film-only finish.
Outdoor stainless railing near saltType 316L with a smooth finishDe-icing salt stains 304, and smooth finishes stain less.
Structural steel outdoorsHot-dip galvanizing, or a zinc-rich paint system if it will not fit a kettleBoth put zinc against the steel.
Animal enclosures and washdown areasGalvanized carbon steel for frames; stainless where it is cleaned constantlyNeither zinc nor stainless depends on an unbroken film.
A rusted look on purposeWeathering steel, only where it can dry, away from salt, with a plan for runoffThe protective layer needs wet and dry cycles.
Light weight matters more than strength at the weldsAluminum, designed around the weld zonesOne-third the weight of steel, weaker beside welds.

If you are not sure which of these your job is, tell us where it is going and what it has to look like, and we will talk it through before we quote. Get in touch.

Common Questions

Is galvanizing or powder coating better for outdoor steel?

They protect in different ways. Galvanizing is a zinc layer that protects the steel even where it is scratched, and the American Galvanizers Association puts its life at 70 years or more in most atmospheres. Powder coating is a sealed film that gives color and a smooth finish, but it only protects while the film is unbroken. Where both long life and color matter, the two are used together.

How long does hot-dip galvanizing last?

The American Galvanizers Association says properly specified hot-dip galvanized steel can provide 70 years or more of maintenance-free protection in most atmospheres, depending on temperature, humidity, pollution and salt in the air. Life is in direct proportion to the zinc thickness, and thicker steel takes on a thicker coating.

Should I use 304 or 316 stainless steel?

Type 316 is Type 304 with 2 to 3 percent molybdenum added, which helps it resist chlorides. The International Molybdenum Association says that within five to ten miles of a large body of salt water, or where the steel is exposed to de-icing salt, Type 316 is often the most cost effective choice if corrosion-free performance is wanted. De-icing salt causes at least surface staining on Type 304.

Can you powder coat or paint over galvanizing?

Yes. The combination is called a duplex system. According to the American Galvanizers Association it can last 1.5 to 2.3 times the combined lifetimes of the two coatings used alone. The zinc surface has to be prepared first, following ASTM D6386 for paint or ASTM D7803 for powder coating.

Does stainless steel rust?

Stainless steel is protected by a thin chromium oxide layer, not by a coating. It can still stain. Salt causes surface staining on the common grades, and bits of carbon steel left on the surface from tools or grinding rust and make the stainless look as if it is rusting. Clean fabrication, a smooth finish and washing all reduce it.

Will weathering steel stain the concrete under it?

It can. Rust runoff staining of surrounding materials is described by the American Galvanizers Association as a major drawback of weathering steel, and the Federal Highway Administration advises protecting the concrete below it.

Sources and Limits

The facts on this page were read from these publishers on November 23, 2026:

  • Galvanizing, duplex systems, and paint and powder as barriers: American Galvanizers Association (galvanizeit.org), including its published tables from ASTM A123 and its ISO corrosion category data.
  • Powder coating: Powder Coating Institute (powdercoating.org).
  • Paint systems and surface preparation: Federal Highway Administration (fhwa.dot.gov), U.S. Bureau of Reclamation, Minnesota Department of Transportation, and the UK steel construction reference steelconstruction.info.
  • Stainless steel: Specialty Steel Industry of North America (ssina.com), British Stainless Steel Association (bssa.org.uk), International Molybdenum Association (imoa.info), and the Australian Stainless Steel Development Association for tea staining.
  • De-icing salt: International Molybdenum Association and The Construction Specifier.
  • Aluminum: Aluminum Extruders Council (aec.org), Aluminum Anodizers Council, U.S. Geological Survey, ESAB for welded strength under AWS D1.2, and Alro Steel for 6061 and 6063.
  • Steel grades: American Institute of Steel Construction, Modern Steel Construction (February 2012), and the Steel Tube Institute (steeltubeinstitute.org). Hot and cold rolled surfaces: Nucor.
  • Weathering steel: Federal Highway Administration technical advisory, American Galvanizers Association, and steelconstruction.info.

Limits. Service life figures are published estimates for general atmospheres, not promises for a particular site. None of the sources gives data for Racine itself; Milwaukee is the nearest city in the galvanizing data. The steel grade preferences come from a 2012 article and the tube industry’s later guidance, which differ on the default tube grade, so we list both. Structural grades and coating systems on an engineered job are set by the engineer and the project specification, and that governs over anything here.

Have a Project?

Talk to Our Team

Our specialists are happy to answer your questions and help scope your project.